Hardening: Heat uniformly to 830/860°C until heated through. Quench in oil or water. Can also be induction or flame hardened.
Tempering: Heat uniformly and thoroughly at the selected tempering temperatures, between 550°C to 660°C and hold at heat for one hour per inch of total thickness.
Normalising: Normalise at 830-860°C, and cool in air.